Our plating Processes JS500 Information
Zinc Plating Phosphate Info
Salt Spray Testing and Results Organics

Salt Spray Results of JS500 Versus

First Run


Mechanical Zinc & Hot Dip Galvanizing

No. of Pcs Checked - 6    Visual Check - OK
Zinc Plating Film Thickness
JS500 - 0.47 mils (Avg)
Mech - 1.25 mils (Avg)
HDG - 1.00 mils (Avg)


Astm B-117

Test Period

1 2
24 48 72 96 120 144 188 192 216 240 264
3 4 5
288 312 338 360 384 408 432 456 480 504

RESULTS:

White rust on Mech & HDG in less than 24 hours.
White rust on JS500 after 168 hours.
Red rust on Mech after 432 hours.
Red rust on HDG after 456 hours.
Parts tested to 1000 hours. JS500 showed NO SIGNS OF RED RUST.

Tests were run and recorded by Jai Balkssoonsingh C.Q.E.
11/18/1992


Second Run


Mechanical Zinc & Hot Dip Galvanizing

No. of Pcs Checked - 6 Visual Check - OK
Zinc Plating Film Thickness
JS500 - 0.37 mils (Avg)
Mech - 2.14 mils (Avg)
HDG - 2.00 mils (Avg)


Astm B-117

Test Period

1 2
24 48 72 96 120 144 188 192 216 240 264
3 4 5
288 312 338 360 384 408 432 456 480 504

RESULTS:

White rust on Mech & HDG in less than 24 hours.
White rust on JS500 after 240 hours.
Red rust on HDG after 648 hours.
Red rust on Mech after 696 hours (1 of 2 Samples).
Red Rust on Mech after 912 on both samples.
No red rust on JS500 after 1200 hrs

Tests were run and recorded by Jai Balkssoonsingh C.Q.E.
11/18/1992